Foaming plastic sheet cross-section produces broken bubble or through the bubble of two factors:
Comprehensive process, price and performance, etc., it is appropriate to mix the two at a certain ratio, the ratio can be 80/20-20/80. Plate forming a wider cross-sectional area, from the extruder head into the mouth of the mould to be distributed to a width equivalent to about 1.3 m. To get fully foamed low-density plastic products, the resin viscosity used should not be too high, in order to facilitate the dispersion of bubbles and expansion, the plate the entire cross-section of the pressure coordinated with the requirements of the melt fluidity. If the PVC resin viscosity is too high, the melt fluidity is poor, it is difficult to ensure the flatness of the plate, the bubble holes are not easy to expand, resulting in a low foaming times; on the contrary, if the PVC resin viscosity is too low, it will lead to the melt strength is low, easy to trigger the bubble.
The production of crust foam plastic sheet should use SC-7 resin, try not to use SC-8 resin, or use SC-8 resin mixed with SC-5 or SC-6 resin.
Good plasticisation of the melt is a prerequisite for foamed plastic sheet products. If there is a problem with the heat stabiliser, the extrusion temperature is too high, the melt is prone to local degradation and will be torn because of the reduction of melt strength, the bubble is too large; extrusion temperature is too low, the melt is not plasticised, the strength is very low, the same will be broken bubble. Foaming plastic sheet production, must be regularly on the stabiliser 180 ~ 200 degrees of stability test, does not meet the stability requirements of the raw material shall not be used or adjust the dose, after passing the test and then use.
In addition to ensure that the melt does not degrade in the extrusion process, the stabiliser also has an important function, that is, to regulate the decomposition temperature of the blowing agent. If the amount of stabiliser is too much or too little, the decomposition temperature of the blowing agent is too low or too high, which is not conducive to foaming. Stabiliser should be adjusted according to the grade of resin used, such as the use of 8-type resin, the plasticising temperature is low, the stabiliser should be increased appropriately, so that the material plasticising temperature and the decomposition temperature of the blowing agent to match. However, if the stabiliser is added too much or the melt temperature is too high, it will lead to early decomposition of the blowing agent in the extruder, resulting in foaming gas escaping from the charging hole and the vacuum hole, if the stabiliser is added too little or the operating temperature is too low, it will make the foaming incomplete.
Extrusion operation, in addition to ensuring good melt plasticisation, the melt temperature in the extruder must be lower than the decomposition temperature of the blowing agent, to prevent the premature decomposition of the blowing agent in the machine; the melt temperature of the exit mould must reach the decomposition temperature of the blowing agent region, in order to facilitate the full foaming. The setting and control of extrusion temperature should also be adjusted in time according to the vacuum hole material and the melt moulding form when the machine is switched on. Ensure that the material through the vent hole is basically orange peel state, the bottom of the screw should not be powder flow; melt extrusion from the mouth of the mould surface should be smooth, with a certain degree of elasticity, shall not be an exit mould on the sagging or cross-section of the crystalline rough.
Foaming plastic sheet production generally use heat type, heat-absorbing type or heat-absorbing, exothermic composite balance of three different blowing agents. Ammonium azodicarboxylate, also known as AC, belongs to the azodyne activator, AC foaming agent decomposition temperature is high, up to 232 degree , far beyond the PVC processing temperature, the use of decomposition temperature needs to be reduced.
Exothermic foaming agent foaming rate is high, about 190-260ml/g, decomposition speed, exothermic great, but the foaming time is short, suddenness is also strong. Therefore, when AC blowing agent dosage is too much, the amount of gas generation is too large, it will make the pressure inside the bubble grow fast, the size of the bubble hole grows too large, the gas is released sharply, so that the structure of the bubble hole is damaged, the size of the bubble hole is not evenly distributed, and even the formation of the open hole structure, which will produce large bubbles and cavities in the local area.
Production of foamed plastic products, exothermic blowing agent AC shall not be used alone, should be used in conjunction with heat-absorbing blowing agent or the use of heat and exothermic balance of composite chemical blowing agent. Inorganic foaming agent - sodium bicarbonate (NaHCO3) is a heat-absorbing foaming agent, although the foaming rate is low, but the foaming time is long, and AC-type foaming agent mixed, can play a complementary and balanced role. Exothermic foaming agent to improve the heat-absorbing foaming agent of the gas generating capacity, heat-absorbing foaming agent and the former cooling, stabilising its decomposition and balanced release of gas, inhibit overheating degradation of the interior of the thick plate to reduce the precipitation of residues, there is a whitening effect.
Under the premise of not affecting the foaming rate, it is appropriate to add more heat-absorbing blowing agent to replace some of the exothermic blowing agent, in order to inhibit the addition of exothermic blowing agent triggered by the breakage of the bubble.1232 or BLA-616 blowing agent is an exothermic and heat-absorbing balanced blowing agent, decomposition of the non-inductive period, the rate of decomposition is fast, 10 minutes or so to reach the maximum amount of gas, slow deflation, no bursts of gas, the maximum amount of gas up to 156mL. Its decomposition temperature between the PVC processing temperature range, can be used for the size of thicker, complex shape of the product dynamic moulding process, in order to eliminate the broken bubbles, to ensure the stability of foaming performance.
It should be pointed out that the molecular weight and viscosity of foam regulator produced by different manufacturers are very different, when the foam products have broken bubbles or cascade bubbles, and other methods of treatment is ineffective, a separate replacement of the foam regulator or an appropriate increase in dosage, will often produce significant results. However, increasing or replacing the foaming regulator with larger molecular weight will increase the density of the product because the viscosity is too large, which makes the air bubbles in the melt unable to expand. And because of the viscosity of the melt is too large, the fluidity becomes poor, resulting in the mouth of the mould out of the material is not uniform, affecting the flatness of the board, and even production time is not long, the mouth fuzzy material failure occurs, especially when the production of 10mm thick or less than the plate is more likely to occur.
Production of different thicknesses of the plate, the processing regulator dose should be different depending on the situation, the same formula, thin plate without bubble holes, thick plate bubble holes, it is appropriate to add more 0.3-0.5 parts of the processing regulator, only to eliminate the bubble as the basis for micro-additive, do not recklessly, blindly add more, so as not to increase the density of the product, affecting the effective production time.
CaCO3 add too much, although it can form more bubble nuclei, but if the calcium carbonate add too much or too large a particle, the activity is not good, the formation of agglomerates, dispersed in the resin or resin cross-section with a bad combination, resulting in a reduction in the strength of the melt, the melt is easy to produce bubble expansion bubble.
Ⅷ. plate cross-section foaming or uneven material, local lack of material.
Sheet cross-section foam or uneven material, local lack of material affects more factors, throughout the mixing and extrusion of the whole process. For example, the formula components are not reasonable, the outer slip is too little, the temperature of the extruder 5 area is easy to overheat, resulting in high temperature of the combined core, the middle of the plate appeared large bubbles, string bubbles, yellowing, plate surface roughness and other defects; single pot mixing amount is too much, the mixing temperature is too low, mixing time is too short, the inner slip is added too little, easy to lead to the mixture of components dispersed unevenly.